245 0 0 _aEffect of water on steel corrosion under supercritical CO2 conditions
260 _a
_b
_cjun. 2011
270 _a01/07/2011 ; 01/07/2011
300 _a7 p. ; 62-68
520 _aTranscripción del resumen del autor. Rotating cage corrosion experiments were performed on two carbon steels (CS) and three stainless steels (SS) in supercritical carbon dioxide (SC CO2) and different amounts of water at 50, 80, 110, and 130 °C. Water phases in equilibrium with SC CO2 cause high corrosion rates on CS (5 to 15 mm/y) but only 0.3 to 0.8 mm/y on 13Cr SS. Duplex SS and austenitic CrNi SS were <0.1 mm/y at 110 °C.